Figures
Abstract
The internal pressure strength of tubing and casing often cannot satisfy the design requirements in high pressure, high temperature and high H2S gas wells. Also, the practical safety coefficient of some wells is lower than the design standard according to the current API 5C3 standard, which brings some perplexity to the design. The ISO 10400: 2007 provides the model which can calculate the burst strength of tubing and casing better than API 5C3 standard, but the calculation accuracy is not desirable because about 50 percent predictive values are remarkably higher than real burst values. So, for the sake of improving strength design of tubing and casing, this paper deduces the plastic limit pressure of tubing and casing under internal pressure by applying the twin shear unified strength theory. According to the research of the influence rule of yield-to-tensile strength ratio and mechanical properties on the burst strength of tubing and casing, the more precise calculation model of tubing-casing's burst strength has been established with material hardening and intermediate principal stress. Numerical and experimental comparisons show that the new burst strength model is much closer to the real burst values than that of other models. The research results provide an important reference to optimize the tubing and casing design of deep and ultra-deep wells.
Citation: Lin Y, Deng K, Sun Y, Zeng D, Liu W, Kong X, et al. (2014) Burst Strength of Tubing and Casing Based on Twin Shear Unified Strength Theory. PLoS ONE 9(11): e111426. https://doi.org/10.1371/journal.pone.0111426
Editor: Yogendra Kumar Mishra, Institute for Materials Science, Germany
Received: May 31, 2014; Accepted: August 8, 2014; Published: November 14, 2014
Copyright: © 2014 Lin et al. This is an open-access article distributed under the terms of the Creative Commons Attribution License, which permits unrestricted use, distribution, and reproduction in any medium, provided the original author and source are credited.
Data Availability: The authors confirm that all data underlying the findings are fully available without restriction. All relevant data are within the paper.
Funding: This work was supported by National Natural Science Foundation of China (No. 51274170) to LYH. The funders had no role in study design, data collection and analysis, decision to publish, or preparation of the manuscript.
Competing interests: The authors have declared that no competing interests exist.
Introduction
In “three-high” (high pressure, high temperature, and high H2S) gas wells, the service environment of tubing and casing becomes more complicated and harsh, and the internal pressure applied to tubing and casing becomes higher. Hence, the tubing and casing must have adequate burst strength to withstand the internal pressure without deformation. Furthermore, gas channeling and overflow may occur in case of burst of tubing and casing in “three-high” gas wells, which results in serious consequences [1]. Many scholars have done studies on strength of tubing and casing as the tubing and casing play an important role in the process of wellbore integrity, and many new methods and models (such as yield failure model, plastic collapse failure model and crack propagation model) which were used to analyze the strength of tubing and casing have been created [2]–[5]. But most of them only can predict the burst strength of thin-walled high-strength pipeline used to transport crude oil above the ground [6]–[7] instead of thick-walled tubing and casing underground.
However, the study on the API 5C3 strength model has found that the model can only predict the minimum internal pressure strength of tubing and casing. The basic failure criterion of API 5C3 depends on the initial yield of inner wall surface under the internal pressure, yet the casing has the ability of seal integrity and structure integrity in this situation. So, many tubular products were wasted in conventional wells and the tubing and casing strength often cannot satisfy the design requirement in rigorous wells (such as “three-high” gas wells) according to the current API 5C3 standard [8].
In addition, the initial yield in inner wall surface can't be presented in test or practical field. On the contrary, burst can truly reflect the loss of seal integrity in tubing and casing. Accordingly, ISO 10400:2007 [9] has proposed burst strength (ductile rupture strength) of tubing and casing and offered the model to calculate the burst strength of pipe (tubing and casing) under internal pressure. Compared with API 5C3 standard, the ISO burst strength model can predict the burst strength of tubing and casing according to the minimum wall thickness much better [10]–[12] and improve the design of tubing and casing strength to some extent. But, the study on the ISO strength model has found that its calculation precision is not desirable since approximately 50 percent predictive values are remarkably higher than real burst values [13]–[14], which goes against the design of tubing and casing strength and the improvement of upper limit of safety factor in the well Long-gang-001-1, Long-gang-001-2, Long-gang-13, Pu-guang-204-2H in Sichuan and Chongqing gas fields and the well Yingshen-1 in Tarim oilfield as well as the well TK1127 in Tahe oilfield in Xinjiang.
Moreover, in oil and gas industry, the tubing is the key component for transporting crude oil and gas, and the casing plays an important role in protecting and reinforcing borehole, isolating oil, gas and water during drilling and production. As a result, in order to improve the strength design of tubing and casing, on the basis of my work group results [13]–[14], based on the twin shear unified strength theory and twin shear stress yield criterion [15]–[16], the model that can calculate the burst strength of tubing-casing has been presented under capped-end conditions in this paper. Lots of numerical and experimental comparisons show that the prediction accuracy of “new burst strength model” is higher than that of ISO, and it can meet the requirement of engineering design of deep and ultra-deep wells.
Mathematical Modeling
API 5C3 internal pressure strength model
The model, which can calculate the minimum internal pressure strength of tubing and casing, has been presented by API Bulletin 5C3 [8] based on the yield design criterion by the following expression:(1)where D is the outer diameter of pipe, mm; σy is the yield strength of pipe, MPa; and kwall is the factor to account for the specified tolerance of the pipe wall. For example, for a tolerance of minus 12.5%, kwall = 0.875; PiR-API is the internal pressure strength calculated by Eq. (1), MPa; and t is the specified pipe wall thickness, mm.
For the API 5C3 strength model, the basic principle of yield caused by internal pressure is that initial yield in inner surface of pipe is failure, yet without loss of pressure/seal integrity. Initial yield in inner surface can't be presented in test or practical field. However, the pipe burst can truly reflect the loss of pressure/seal integrity in casing.
ISO burst strength model under capped-end conditions
The yield design criterion can only meet the minimum design standard, and the API 5C3 model could not predict accurately the maximum load of tubing and casing. As a result, the ISO burst strength model under capped-end conditions has been proposed by Klever and Stewart [17]–[18]:(2)where n is the dimensionless hardening exponent used to obtain a curve fit of the true stress-strain curve derived from the uniaxial tensile test (see ISO 10400: 2004 [9]), σuts is the tensile strength of specimen, MPa; and PiR-iso is the burst strength calculated by Eq. (2), MPa.
The research on the ISO burst strength model has found that it can better predict the burst strength of tubing and casing by using the minimum wall thickness of pipe than API 5C3 [10]–[12]. However, it can be observed from the 106 groups of test data provided by three industry sources [9] that 50 percent predictive values of ISO burst strength model are remarkably higher than real burst values, which points against the design of tubing and casing strength and the improvement of upper limit of safety factor. Hence, the current ISO burst strength model cannot be used to predict precisely the burst strength of tubing/casing, which is not the purpose to propose the ISO burst strength model for the joint API/ISO work group ISOTC67 SC5 WG2b.
New burst strength model of tubing and casing
(1) Twin shear unified strength theory.
The twin unified strength theory can be transformed into many strength criterions (such as Tresca yield criterion, Von-Mises yield criterion and twin shear stress yield criterion) and some new criterions according to specific conditions [15]–[16], and it could be used to analyze limit load of various materials because the effects of intermediate principal stress and tensile/pressure ratio (the ratio of tensile strength to compressive strength) of material on the limit load have been taken into account. The mathematical expression of twin shear unified strength theory can be given as follows:(1)(2)wherewhere σ1, σ2 and σ3 are the first, second/intermediate and third principal stress respectively, MPa; α is the tensile/pressure ratio; σt is the tensile strength, MPa; σc is the compressive strength, MPa; τs is the shear strength, MPa; b is the influence coefficient which reflects the effect of second/intermediate principal stress on the material failure.
(2) Elastic limit analysis of tubing and casing under internal pressure.
The stress components (radial stress σρ and circumferential stress σθ) of the tubing and casing increase with the increase of internal pressure P, as shown in Figure 1. The tubing and casing will be in the elastic limit state, when the inner wall yields firstly. Assume that the tubing and casing is a long thick-walled cylinder. In Figure 1, R is the outer radius; r is inner radius; P is the internal pressure at the inner surface of pipe. The long thick-walled cylinder is in the elastic state, when the internal pressure (P) is lower. According to the Lame formula [19], the following stress components can be obtained:(3)
The mechanical analysis of long thick-walled cylinder under internal pressure is one of the axisymmetric plane strain problem. According to the study on the plane strain problem [20]–[21], the intermediate principal stress (, where m = 1) can be obtained in the elastic limit state of pipe. By the Eq. (3), Eq. (4) can be given:(4)
Based on the stress state of thick-walled cylinder, it could be known that the first, second and third principal stress (σ1, σ2 and σ3) are equal to σθ, σz and σρ respectively due to . So the intermediate principal stress (σ2) is smaller than because the tensile/pressure ratio (α) is less than 1.0. Substituting Eq. (3) and Eq. (4) into Eq. (1) gives:(5a)
To analyze the plastic limit load of thick-walled cylinder conveniently, the Eq. (5a) is simplified into Eq. (5b).(5b)
The inner wall of thick-walled cylinder yields firstly, when the internal pressure increases to the yield strength of the material. By the Eq. (5), the elastic limit load (Py) can be obtained:(6)where the Py is the elastic limit load (internal pressure strength), MPa; σs is the yield strength of tubing and casing, MPa.
(3) Plastic limit analysis of tubing and casing under internal pressure.
The plastic region will be formed near the inner wall of thick-walled cylinder, when internal pressure (P) is larger than elastic limit load (Py). Assume that Rc is the radius of interface between elastic region and plastic region, mm, as shown in Figure 1. The plastic region will extend from inner surface to outer surface with the increase of internal pressure (P), which will result in the range of becoming plastic region and the range of becoming elastic region, as shown in Figure 1.
The interface between the elastic region and plastic region is cylinder surface due to the axial symmetry of stress components (σθ and σr). Assume that the elastic region is an outer cylinder, as shown in Figure 2, and the plastic region is an inner cylinder, as shown in Figure 3. Therefore, the elastic and plastic regions are analyzed based on the principle of long thick-walled cylinder. According to axial symmetry, the radial pressure (q) is applied to outer wall of inner cylinder and inner wall of outer cylinder respectively, as shown in Figure 2 and Figure 3.
In plastic region (), as shown in Figure 3, based on the equilibrium equation of plastic mechanics [19], the Eq. (7) can be obtained:(7)
By the Eq. (3) and Eq. (5b), the Eq. (8) can be obtained:(8)
Substituting Eq. (8) and boundary conditions () into Eq. (7) gives:(9a)(9b)
In elastic region (), as shown in Figure 2, according to the lame formula, the stress components can be obtained:(10)where(11)
According to continuity of the radial stress (), the radial stress of elastic region is equal to plastic region at the interface (). As a result, by the Eq. (9a), Eq. (10) and Eq. (11), the Eq. (12) can be obtained:(12)where
The plastic region increases with the increase of internal pressure (P). The whole wall of thick-walled cylinder is in plastic state, when the radius of interface (Rc) is equal to the outer radius (R) of thick-walled cylinder. According to the Eq. (12), the plastic limit load (Pp) can be obtained:(13)
Based on the twin shear yield criterion, by the Eq. (13), the burst strength model can be obtained:(14)
The Eq. (14) used to calculate burst strength of real tubing and casing based on the yield strength (σs) of tubing and casing is not reasonable and needs to be further improved because the real tubing and casing will undergo the hardening stage and large plastic deformation from inner wall yield to whole wall yield. Hence, the yield strength (σs) of tubing and casing has been replaced by flow stress (σf) to calculate the burst strength accurately and reasonably in this paper. The Klever's research results [17] also demonstrated that the flow stress (σf) which can deal with the effect of hardening and larger plastic deformation on the burst strength of tubing and casing ranged between the yield strength and tensile strength. In addition, for the different metal pipe, some empirical formulas of flow stress have been proposed by some scholars [22]–[24], as follows:(15)
The study on the Eq. (15) has indicated that the yield-to-tensile strength ratio (the ratio of yield strength to the tensile strength) has a great effect on the burst strength of tubing and casing. Especially, for the lower the yield-to-tensile strength ratio and, smaller the yield-to-tensile strength ratio, the capacity for plastic deformation is higher [25], which is in agreement with my work group results [26]. So, on the basis of results of our work group [13]–[14], a new burst strength model (Eq. (16)) for predicting the burst strength of tubing and casing under capped-end conditions is presented with consideration of the yield-to-tensile strength ratio, manufacturing imperfection (including the ovality and eccentricity of pipe), crack defects (the crack depth of pipe), material hardening (the phenomenon that the material strength and hardness increase in the process of plastic deformation [27]) etc.:(16)where tdc = t-aka, a is the crack depth that should be less than 5% of the wall thickness, mm; ka is the burst strength factor, having the numerical value 1, 0 for quenched and tempered (Martensitic structure) or 13Cr products and 2, 0 for as rolled and normalized products based on available test data; and the default value set to 2, 0 where the value has not been measured [9].
The new burst strength model (Eq. (16)) could predict burst strength of tubing and casing accurately and reasonably, which will make great improvements in the tubing and casing design of deep and ultra-deep wells on the basis of material safety which was guaranteed.
Results and Discussion
In order to validate the accuracy and reliability of the new burst strength model (Eq. (16)), the calculation results of the new model have been compared with the calculation results of the API model [8], ISO model [9], Nadai model [28] and the 106 groups of experiment data (PiR-test) donated from three industry sources under capped-end conditions due to the high internal pressure [9]. The comparisons of calculation results and experiment data are shown in Figure 4. In Figure 4, the x-coordinate is the ratio of experiment data (PiR-test) to calculation results of model; the y-coordinate is number of the data; PiR-ISO is the burst strength calculated by the ISO model; PiR-New is the burst strength calculated by the new model; PiR-API is the burst strength calculated by the API model; PiR-Nadai is the burst strength calculated by the Nadai model.
From Figure 4, the following may be noted.
For the 106 groups of ratio of PiR-test/PiR-New, 75 groups (70.8%) fall in the closed interval [1.0–1.1]; 13 groups (12.3%) fall in the closed interval [1.1–1.2]; and only 18 groups (16.9%) fall in the closed interval [0.9–1.0]. For the 106 groups of ratio PiR-test/PiR-ISO, 50 groups (about 50%) of calculation are higher than the test data. For the 106 groups of ratio PiR-test/PiR-API, all the ratios are considerably larger than 1.2, which demonstrates all the calculations are considerably less than test data. For the 106 groups of ratio PiR-test/PiR-Nadai, all the ratios are considerably smaller than 1.0, and 55.6 percent of the calculations are 20 percent larger than test data.
To validate the accuracy of the new model, the calculations of burst strength for the 16 kinds of frequently-used casing (7<D/t<26) have been presented in Table 1. In general, it can be observed from Table 1 that the calculations of model are PiR-API<PiR-New<PiR-ISO<PiR-Nadai. It can be seen from Figure 5 that PiR-API is considerably less than the test data; PiR-Nadai is considerably larger than the test data; PiR-ISO is close to the test data, but its calculations is almost larger than the test data, which makes against the casing design and improvement of upper limit of safety coefficient. However, PiR-New is quiet closer to the test data and its calculations are only slightly less than the test data (to meet the requirement of engineering design, the calculations must be less than real values, but not 10 percent less than real values), which is beneficial to casing design of deep and ultra-deep wells and improvement of upper limit of safety coefficient on the basis of material safety which was guaranteed. So the new model is more accurate and reasonable than other models.
The new model is more accurate and beneficial to design burst strength of the tubing and casing and improves the upper limit of safety coefficient than other models according to the numerical and experimental comparisons. The design principal of API model is so conservative that the internal pressure strength has a large margin when the inner wall of pipe yields. The Nadai model calculates the burst strength of pipe by using the tensile strength directly without consideration of material hardening so that the calculations are obviously larger than test. The calculations of ISO model is close to test data with consideration of material hardening, but it could overestimate the limit loads and give unsafe predictions for tubing and casing, which is detrimental to the design of real tubing and casing and the increase proves the upper limit of safety coefficient to some degree.
The study results could provide references for the study on the impact of tensile/pressure ratio (the ratio of tensile strength to compressive strength) [29] on the internal pressure strength. For three high gas wells, the study of my work group [30] shows the failure mode belongs to crack expansion instability, when the crack depth is more than 5% of the wall thickness. The tubing and casing should be designed by combining the theory of fracture mechanics and strength theory.
Conclusions
For the sake of improving the calculation and design accuracy of API and ISO standard, based on the twin shear unified strength theory and twin shear stress yield criterion, a new burst strength equation has been presented with due consideration of manufacturing imperfections, yield-to-tensile strength ratio, crack defects, material hardening and intermediate principal stress in its calculation so that the new model can better reflect actual mechanical properties of the tubing and casing and improve the burst strength calculation accuracy.
Numerical and experimental comparisons show that the calculation accuracy of Eq. (16) is better than that of API and ISO. Hence, the Eq. (16) can be used as the lower bound design equation, which will make great improvements in “three high” gas wells tubing and casing designs, rather than just using API bulletin 5C3 or ISO because not only does it avoid the material loss but also guarantees the safety and reliability of material.
Acknowledgments
Authors are thankful for the financial assistance provided by the National Natural Science Foundation of China (No. 51274170).
References
- 1. Yongxing S, Yuanhua L, Ping L, Xiangdong S, Hongbin L, et al. (2010) Burst Design of Casing and Tubing String Using ISO10400. Petroleum drilling techniques 38: 67–69.
- 2. Aasen JA, Aadnoy BS (2007) Three-dimensional well tubular design improves margins in critical wells. Journal of Petroleum Science and Engineering 56: 232–240.
- 3. Deli G, BaoKui G (2004) A method for calculating tubing behavior in HPHT wells. Journal of Petroleum Science and Engineering 41: 183–188.
- 4. Kamaya M, Suzuki T, Meshii T (2008) Failure pressure of straight pipe with wall thinning under internal pressure. International Journal of Pressure Vessels and Piping 85: 628–634.
- 5. Hasan S, Khan F, Kenny S (2012) Probability assessment of burst limit state due to internal corrosion. International Journal of Pressure Vessels and Piping 89: 48–58.
- 6. Law M, Bowie G (2007) Prediction of failure strain and burst pressure in high yield-to-tensile strength ratio linepipe. International journal of pressure vessels and piping 84: 487–492.
- 7. Lizhong W, Yongqiang Z (2011) Plastic collapse analysis of thin-walled pipes based on unified yield criterion. International Journal of Mechanical Sciences 53: 348–354.
- 8.
Committee on Standardization of Tubular Goods (1994) Bulletin on formulars and calculations for casing, tubing, drill pipe and line properties. America Petroleum Institute. 60 p.
- 9.
ISO Technical Committees (2007) Petroleum and natural gas industries-Formulae and calculation for casing, tubing, drill pipe and line pipe properties. International Organization for Standardization. 304 p.
- 10.
Paslay PR, Cenocky EP, Wink R (1998) Burst Pressure Prediction of Thin-Walled, Ductile Tubulars Subjected to Axial Load. SPE: 48327. Available: https://www.onepetro.org/search?q=48327. Accessed 10 July 1998.
- 11.
Stewart G, Klever FJ (1998) Accounting for Flaws in the Burst Strength of OTCG. SPE: 48330. Available: https://www.onepetro.org/conference-paper/SPE-48330-MS. Accessed 7 May 1998.
- 12.
Tallin AG, Paslay PR (1998) The Development of Risk-Based Burst Design for Well Casing and Tubing. SPE: 48320. Available: https://www.onepetro.org/conference-paper/SPE-48320-MS. Accessed 7 May 1998.
- 13.
Yongxing S (2008) Study on Collapse Strength and Internal Pressure Strength of Casing and Tubing, electronic journal. Ph.D. Thesis, Southwest Petroleum University. Available: http://lib.Swpu.edu.cn/paperx/paper_005369.html. Accessed 10 July 2016.
- 14.
Lin W (2010) Study on the internal pressure strength of casing. M. Sc. Thesis, Southwest Petroleum University, Sichuan. Available: http://lib.swpu.edu.cn/paperx/paper_006504.html. Accessed 10 July 2013.
- 15.
Maohong Y (2004) Unified strength theory and its applications. Berlin: Springer. 412 p.
- 16. Jianjun F, Junyan Z, Ping Z, Lifen H (2004) Plastic limit load analyses of thick walled tube based on twin shear unified strength theory. Acta mechanica solida sinica 25: 208–212.
- 17.
Klever FJ (1992) Burst strength of corroded pipe: “Flow stress” revisited. SPE: 7029. Available: https://www.onepetro.org/conference-paper/OTC-7029-MS. Accessed 4 May 1992.
- 18.
Klever FJ, Stewart G (1998) Analytical Burst Strength Prediction of OCTG With and Without Defects. SPE: 48329. Available: https://www.onepetro.org/conference-paper/SPE-48329-MS. Accessed 8 May 1998.
- 19.
Zhilun X (2006) Elasticity Mechanics (The fourth editon). Beijing: Higher Education Press. 308 p.
- 20. Maohong Y, Songyan Y, Chunyang L (1997) Unified plane-strain slip line field theory system. China civil engineering Journal 30: 182–185.
- 21. Lee YK, Ghosh J (1996) The significance of J3 to the prediction of shear bands. International Journal of Plasticity 12: 1179–1197.
- 22. Xiankui Z, Brian NL (2005) Influence of yield to tensile strength ratio on failure assessment of corroded pipeline. Journal of pressure vessel technology 127: 436–442.
- 23.
American National Standards Institute (1984) Manual for Determining the Remaining Strength of Corroded Pipelines, ASME Guide for Gas Transmission and Distribution Piping Systems B31G. American Society of Mechanical Engineers.
- 24.
Kiefner JF, Vieth PH (1989) A Modified Criterion for Evaluating the Remaining Strength of Corroded Pipe, Pipeine Research Committee Report PR3–805. Available: http://www.osti.gov/scitech/biblio/7181509. Accessed 22 Dec 1998.
- 25. Shunhu Z, Dewen Z, Xiaonan W (2014) Influence of yield-to-tensile strength ratio (Y/T) on failure assessment of defect-free and corroded X70 steel pipeline. Journal of Central South University 21: 460–465.
- 26. Yuanhua L, Yongxing S, Taihe S, Kuanhai D, Liexiang H, et al. (2013) Equations to Calculate Collapse Strength for High Collapse Casing. Journal of Pressure Vessel Technology 135: 0412021–5.
- 27.
Jianan W (1980) Metallography and Heat Treatment. Beijing: China Machine Press. 1980. 345 p.
- 28.
Nadai A (1931) plascity. McGraw-Hill. 349 p.
- 29. Junhai Z, Yan L, Changguang Z, Jianfeng X, Peng W (2013) Collapsing strength for petroleum casing string based on unified strength theory. Acta Petroleum Sinica 34: 969–976.
- 30. Yongxing S, Taihe S, Yuanhua L, Zhongsheng W, Zhibin W, et al. (2009) Prediction of Burst Strength of Oil Well Casing Strings with Micro-Cracks. Petroleum Drilling Techniques 37: 35–38.